TABLE I

Average Gas Flow Measurements through Microchannels Laser Drilled into the PE and EVA Film Patches; the Measurement Was Performed at a Pressure Difference between 50 mbar and 1000 mbar

 Flow Rate (mL/Min)
Differential Pressure (mbar)501003005007001000
Nominal Leak Size (µm)EVA Film 300 µm
 20.0100.0170.0410.0710.1020.144
 150.2200.4341.2521.9372.6263.559
 200.4320.8452.2493.4524.6106.099
 301.6662.7796.2009.05011.60514.219
 507.33011.97523.27532.53440.91449.832
 10031.96448.80494.278130.394163.300211.104
 EVA Film 360 µm
 20.0110.0140.0350.0640.0950.119
 5 0.0230.0900.1590.2440.296
 150.2930.5931.6282.5533.4664.665
 200.4330.8472.3143.5924.7816.431
 301.0021.8364.4156.4988.26910.658
 508.24612.37426.33036.96446.61658.893
 10033.40551.53999.794137.903173.022222.560
 PE Film 400 µm
 20.0090.0170.0450.0750.1120.171
 5 0.0290.1180.1860.2580.370
 150.2290.4381.3021.9572.6483.628
 200.3640.6941.9202.9463.9425.363
 300.7251.4373.4065.0576.4148.283
 506.71310.84321.69530.18737.70848.176
 10031.24947.86790.866124.468153.042193.910
  • EVA = ethylene vinyl acetate; PE = polyethylene.